Stainless steel grade guide for buyers
Most grade arguments are really two questions: how much chloride is in the service environment, and how hot does it get. Everything else — price, weldability, availability — follows from those two answers. This page gives the numbers behind the choice, so you can check a supplier's recommendation instead of accepting it.
The grades we stock and what separates them
| Grade | Approx. composition | PREN | Service note |
|---|---|---|---|
| 201 | 16–18% Cr, 3.5–5.5% Ni, 5.5–7.5% Mn | ≈15–17 | Cheapest option; indoor and dry service only — it stains and pits sooner than 304 outdoors or near the coast |
| 301 | 16–18% Cr, 6–8% Ni | ≈17–19 | Work-hardens fast; used for springs, clips and parts needing high strength after forming |
| 304 / 304L | 18% Cr, 8% Ni (L: max 0.03% C) | ≈18–20 | The general-purpose grade. Adequate for food, water, indoor architecture; marginal in coastal air |
| 310S | 25% Cr, 20% Ni | ≈22–25 | High-temperature service; oxidation resistance well above 304, low strength at temperature |
| 316 / 316L | 16–18% Cr, 10–12% Ni, 2–3% Mo (L: max 0.03% C) | ≈24–26 | The default for chlorides, marine air, chemical and medical service |
| 321 | 18% Cr, 9–12% Ni, Ti stabilised | ≈18–20 | Stabilised against sensitisation; cyclic service around 400–900 °C, exhaust and heat exchangers |
| 347 | 18% Cr, 9–12% Ni, Nb stabilised | ≈18–20 | Same idea as 321 with niobium; preferred where welding is heavy or service is continuous at temperature |
| 630 / 17-4PH | 17% Cr, 4% Ni, 4% Cu, Nb | ≈17 | Precipitation hardening; high strength after ageing, used for machined parts, shafts and valves |
| 904L | 20% Cr, 25% Ni, 4.5% Mo, 1.5% Cu | ≈34–36 | High-alloy austenitic for sulfuric and phosphoric acid service; expensive, and worth it only where 316 fails |
PREN — pitting resistance equivalent number — is calculated as Cr + 3.3 × Mo + 16 × N. It is a ranking tool, not a guarantee: it predicts relative resistance to pitting, not to stress corrosion cracking, and it says nothing about acids. Use it to compare 304 against 316 (≈19 vs ≈25) and 316 against 904L (≈25 vs ≈35), not to certify a service.
Choosing by environment
| Service | Start with | Step up when |
|---|---|---|
| Indoor equipment, dry, cleaned with mild detergents | 304 or 201 | Cleaning chemicals contain chloride |
| Food and beverage contact, hygienic finish | 304, 316L for dairy and brine | Product contains salt or chloride sanitisers |
| Coastal or marine atmosphere, unwashed | 316L | Welded and not post-weld cleaned — consider 2205 or 904L |
| Heat exchanger, chlorinated cooling water | 316L | Chloride above roughly 200 mg/L or temperature above 60 °C |
| High temperature, cyclic, 400–900 °C | 321 or 347 | Continuous service — 347 or a higher alloy |
| Sulfuric or phosphoric acid | 904L | Concentration and temperature decide; check a corrosion chart, not a grade name |
| Machined parts needing strength | 630 (17-4PH) | Corrosion dominates over strength — back to 316L |
Equivalent designations
| ASTM / UNS | EN | JIS | GB |
|---|---|---|---|
| 304 / S30400 | 1.4301 | SUS304 | 06Cr19Ni10 |
| 304L / S30403 | 1.4307 | SUS304L | 022Cr19Ni10 |
| 316 / S31600 | 1.4401 | SUS316 | 06Cr17Ni12Mo2 |
| 316L / S31603 | 1.4404 | SUS316L | 022Cr17Ni12Mo2 |
| 321 / S32100 | 1.4541 | SUS321 | 06Cr18Ni11Ti |
| 347 / S34700 | 1.4550 | SUS347 | 06Cr18Ni11Nb |
| 310S / S31008 | 1.4845 | SUS310S | 06Cr25Ni20 |
| 630 / S17400 | 1.4542 | SUS630 | 05Cr17Ni4Cu4Nb |
| 904L / N08904 | 1.4539 | SUS890L | 015Cr21Ni26Mo5Cu2 |
| 201 / S20100 | 1.4372 | SUS201 | 12Cr17Mn6Ni5N |
When a specification names a JIS or GB grade, quote the ASTM or EN equivalent alongside it on the purchase order. Two designations for the same material is the single most common source of a wrong delivery.
Questions buyers ask about grades
What is the difference between 304 and 316?
316 adds 2–3% molybdenum and 2–4 points more nickel. That raises pitting resistance (PREN ≈25 versus ≈19) and is why 316 is the default in chloride and marine service. In dry indoor service the difference rarely justifies the price.
Is 316L better than 316?
316L caps carbon at 0.03% instead of 0.08%, which reduces sensitisation — chromium carbide precipitation at grain boundaries — after welding. For welded assemblies over about 6 mm, L is the safer specification.
Can 304 be used outdoors near the ocean?
It can, and it will stain. Marine air carries chloride; 304 pits and develops tea staining, especially on unwashed horizontal surfaces and at welds. 316L is the minimum for coastal service.
When should I specify 321 instead of 304?
When the part runs cyclically between roughly 400 and 900 °C. Titanium stabilises the carbon so chromium carbides do not form during service. Below that range 304 is fine; above it, 310S or a nickel alloy is the next step.
Is 904L worth the price?
Only where 316 fails. 904L carries about 20% chromium, 25% nickel, 4.5% molybdenum and 1.5% copper, with a PREN around 35. In sulfuric and phosphoric acid service that matters; in seawater piping, 2205 duplex usually does the job at lower cost.
What is 17-4PH used for?
Precision machined parts that need strength: shafts, valve stems, fasteners, pump components. It is supplied annealed and hardens by ageing — typically to H900, H1025 or H1150 conditions, which trade strength against toughness.
Is 201 a real stainless grade or a cheap substitute?
It is a real grade — manganese replaces some nickel — but it is not interchangeable with 304. Corrosion resistance is lower, and it is unsuitable for coastal, wet or chloride-exposed service. It is legitimate for indoor frames and dry decorative work.
What does the L in 304L mean?
Low carbon: 0.03% maximum against 0.08% in standard 304. It matters after welding, where higher carbon can tie up chromium as carbides and leave the grain boundaries vulnerable to intergranular corrosion.
Why did my 304 part pit after six months?
Almost always chloride plus a stagnant surface — salt deposits, cleaning chemical residue, or a weld that was never pickled. Check the environment first: if chloride is present, the grade is the problem, not the batch.
What is the maximum service temperature for 310S?
Roughly 1,100 °C for oxidation resistance in intermittent service, lower for continuous load-bearing service. It resists scaling better than 304 or 316 but has low strength at temperature, so it is a furnace and radiant-tube grade rather than a structural one.
Is 2205 duplex better than 316L?
For chloride stress corrosion cracking, usually yes — duplex is far more resistant. It is also stronger, which allows thinner walls. The trade-offs are welding procedure, limited high-temperature service, and fewer suppliers. Where 316L pits in warm chlorinated water, duplex is the rational step.
Can I use stainless for potable water?
304 and 316L are both widely used in potable water. Chloride level and stagnation decide which: above roughly 200 mg/L, or in warm stagnant lines, 316L is the safer specification.
Does 304 become magnetic?
Cold working — bending, drawing, machining — can make 304 slightly magnetic by transforming some austenite to martensite. A magnet is therefore not a reliable grade test. PMI or a mill certificate is.
Which grade for a brewery or dairy tank?
316L, with a hygienic finish (2B minimum, often 2D or electropolished internally). The concern is chloride sanitisers and cleanability rather than the product itself.
How do I check the grade of material I received?
Positive material identification — X-ray fluorescence or optical emission — on the actual piece, checked against the heat number on the mill certificate. A certificate proves what was melted; PMI proves what arrived.